Results


Summary of CATRA edge retention results on knife blades
Steel Hardness TCC Ratio Source
S125V ? 1200 224 Spyderco
10V 60/61 1044 194 Dozier/Knives Illustrated
S60V 60/61 1030 193 Dozier/Knives Illustrated
S90V 60/61 1014 189 Dozier/Knives Illustrated
20CV ? ? 180 Latrobe
M390 61+ 959 179 Bohler
Elmax 62 931 174 Bohler
T15 65 921 172 Peachy
M4 61 900 168 Bohler
S30V 61 798 149 Bohler
Elmax 60+ 762 142 Bohler
S90V ? 750 140 Spyderco
ZDP-189 ? 750 132 Spyderco
Vanadis 4 Extra 61 709 132 Bohler
S35VN 61 707 132 Bohler
3V 60/61 682 127 Dozier/Knives Illustrated
PM 7.5-1.3-2.75 CrMoV 61 674 126 Bohler
D2 61 666 124 Bohler
154CM ? ? 120 Crucible
N690 61+ 635 118 Bohler
M3 64 586 109 Peachy
S30V 59 565 105 Spyderco
ATS-34 61+ 547 102 Bohler
S30V 60/61 541 101 Dozier/Knives Illustrated
N360 59 536 100 Bohler
440C 59 536 100 Bohler
A2 62 522 97 Peachy
VG-10 ? 505 94 Spyderco
154CM 60/61 468 87 Dozier/Knives Illustrated
O1 64 395 74 Peachy
X15 T.N. 59 354 66 Benchmade
H1 59 172 33 Benchmade